MP159 nickel round bar, MP159 nickel foil, MP159 nickel wire rod, MP159 nickel tube price
▪ UNS R30159
▪ AMS 5841 Bar (Solution Heat Treated)
▪ Solution Heat Treat: 1900°F - 1925°F / 4-8 hours + Water Quench
▪ AMS 5842 Bar (Solution Heat Treated and Work Strengthened)
▪ Solution Heat Treat: 1900°F - 1925°F / 4-8 hours + Water Quench
▪ Followed by work strengthened / strain hardening
▪ AMS 5843 Bar (Solution Heat Treated, Work Strengthened and Aged)
▪ Solution Heat Treat: 1900°F - 1925°F / 4-8 hours + Water Quench
▪ Followed by work strengthened / strain hardening
▪ Followed by ageing: 1200-1250°F 4-4.5 hours + Air Cool.
▪ Landing gears and bolt material
▪ Solid rocket boosters
▪ Jet engines
▪ Chemical processing
▪ Pulp and paper
▪ Power generation equipment
▪ Marine equipment
Element | Content (%) |
Cobalt, Co | 35.7 |
Nickel, Ni | 25.5 |
Chromium, Cr | 19 |
Iron, Fe | 9 |
Molybdenum, Mo | 7 |
Titanium, Ti | 3 |
Niobium, Nb | 0.6 |
Aluminum, Al | 0.2 |
Condition | Tensile Strength ksi | Yield Strength ksi | Elongation % | Reduction of Area % | Hardness HRC |
Annealed | 123 | 58 | 60 | 69 | |
AMS 5841 | 160 max | 70 max | 50 | 65 | 20 HRC max |
Annealed, Cold Worked 48% | 230 | 205 | 12 | 46 | |
AMS 5842 | - | - | - | - | ≥38HRC |
Annealed, Cold Worked + Aged | 275 | 265 | 8 | 35 | |
AMS 5843 | 260 min | 250 min | 6 min | 20 min | ≥44HRC |